Short answer
Bed adhesion comes down to three things: a build surface that suits the material, a first layer printed slowly at the right nozzle height, and a plate free of skin oils. Smooth or textured PEI is enough for PLA in most cases; PETG can bond too strongly to smooth PEI, so use a textured plate or a glue layer as a release agent. ABS and ASA want an enclosure and a brim, and nylon holds best on garolite or a glued engineering plate.
Key takeaways
- The goal is not maximum adhesion but a balance: grip while hot, release once cool.
- Most failures start in the first layer: nozzle height, first-layer speed and a clean plate matter before temperature.
- Skin oil quietly kills adhesion; wipe PEI with isopropyl alcohol when cold and wash it with dish soap now and then.
- Glue does two jobs: it helps weak-bonding materials grip and keeps over-bonding PETG off the coating.
- For warping, fix the environment and first layer first, then add a brim or corner discs.
Why bed adhesion decides the whole print
An FDM print only succeeds while it stays attached to the plate. If the first layer slides, the nozzle prints into thin air; if a corner lifts, the part bends; if the part breaks free halfway through, you come back to a nest of spaghetti. Bed adhesion is less about print quality than about whether there is a print at all.
Yet the right target is not “as strong as possible”. A good surface holds firmly during printing and lets go easily once the plate cools. Too much adhesion is a failure too: PETG tearing chips out of smooth PEI, or a part you can only remove with a scraper, is as frustrating as a part that never stuck.
Four things set that balance: the type of surface, how the first layer is printed, how clean the plate is, and how well the material and surface are matched. We take them in turn below. For a quick path from symptom to cause, see our troubleshooting guide.
Build surfaces: PEI, glass, garolite and more
Most current printers use a flexible spring steel sheet that sits on a magnetic bed. The coating on that sheet is what actually decides adhesion, which means you can change the surface on the same printer simply by swapping plates.
Smooth PEI
PEI (polyetherimide) is a polymer coating that grips many filaments when warm and releases them as it cools. Smooth PEI leaves a glossy, flat underside. Prusa describes its smooth PEI sheet as the best solution for PLA. The same surface can bond too well with PETG, which we return to below.
Textured PEI and powder coatings
On a textured sheet the PEI is sprayed on as a rough layer. The smaller contact area gives a gentler grip, and parts often pop off by themselves once cool. The underside comes out matt and textured, and small scratches disappear into it. For PETG and TPU it is most people's first choice. Fine-textured satin coatings sit between smooth and textured.
Glass
Glass is very flat and hard and gives a mirror-like underside. On its own it grips most materials poorly, usually needs an adhesive and heats slowly. Because it cannot flex, removing a part means waiting for it to cool. It still works on some printers, but spring steel sheets have largely replaced it.
Engineering plates, garolite and PP
Engineering plates are designed for materials that need a hot bed and are usually used with a thin layer of glue. Garolite (G10) is a glass-fibre reinforced epoxy laminate with a good reputation for nylon. Polypropylene (PP) barely sticks to anything, so it is printed on dedicated PP surfaces or PP tape.
| Surface | Strength | Watch out for |
|---|---|---|
| Smooth PEI | Strong grip on PLA, smooth underside | PETG can over-bond; scratches easily |
| Textured PEI | Easy release, good with PETG and TPU | Small PLA parts may need a brim |
| Glass | Very flat, mirror-like underside | Usually needs glue, slow to heat |
| Engineering plate | High-temperature materials | Best used with glue |
| Garolite (G10) | Good grip on nylon | Surface quality varies by supplier |
The first layer: nozzle height, speed and temperature
However good the surface, a badly printed first layer will not hold. Its job is to press molten plastic gently onto the plate so that it forms a wide, flat contact area. How much it is pressed is set by the gap between nozzle and plate.
- Too high: the line stays round, touches the plate along a thin strip and does not merge with its neighbours. The print lifts easily.
- Right: the line flattens slightly, fuses with the next one and the first layer looks even and matt.
- Too low: plastic squeezes out sideways, the surface ripples or gets scraped, the nozzle can score the PEI and the bottom edge flares (elephant's foot).
Modern printers probe the plate, build a height map (mesh) and compensate for small deviations while printing. Automatic levelling helps, but it does not choose the Z offset, the nozzle's zero point, for you. Check the offset again whenever you change plates, especially to a surface of different thickness.
Printing the first layer slowly gives plastic time to settle onto the surface, and running the part fan low for the first layer is common practice. Bed temperature depends on the material: check the product's data sheet for typical ranges. Our print settings guide explains what each setting changes and why.
How to clean a build plate: oils, alcohol and soap
One of the most common causes of poor adhesion, and one of the least suspected, is a fingerprint. The thin film of oil skin leaves behind noticeably weakens how well PEI grips plastic. Hand creams and soaps can leave oils or sugars too, and Prusa warns explicitly that they can ruin adhesion.
- 1
Handle by the edges
Do not touch the print area. Hold the sheet by its edges when fitting and removing it.
- 2
Everyday wipe
With the plate cold, wipe it with high-concentration isopropyl alcohol and a lint-free microfibre cloth. Paper towels can leave fibres behind.
- 3
Occasional deep clean
If alcohol is not enough, wash the sheet with a few drops of dish soap and water, rinse well and dry. Prusa asks for warm rather than hot water for its sheets, while Bambu Lab suggests hot water. Follow your plate maker's instructions.
- 4
Dry and refit without touching
Dry the sheet completely, refit it by the edges and watch the first layer of the next print.
On smooth PEI, marks from the nozzle or tools build up over time. Prusa suggests wiping them gently in circles with the hard side of a dry kitchen sponge. That refreshes the surface a little; it will not bring back deep scratches or a worn-through coating.
Glue: an adhesive and a release agent
Bed glue (usually a PVA-based glue stick or a liquid glue) is used for two opposite jobs, and knowing which one you need clears up a lot of confusion.
- As an adhesive: nylon, PC and some fibre-filled materials grip PEI weakly. A thin layer of glue gives them something to hold on to.
- As a release agent: PETG and flexible filaments can bond too strongly to some surfaces. Glue acts as a buffer between plastic and PEI and stops the coating tearing when the part comes off.
- As protection: Bambu Lab notes that glue makes prints easier to remove and protects the plate surface, the engineering plate in particular.
On its textured sheet, Prusa recommends glue stick as a separation layer for ASA, ABS, nylon and PC blend, while flexible filaments need no glue there. On smooth PEI, it says glue is a must when printing flex. Whatever the case, apply it thin and even: a thick, lumpy layer spoils the first layer.
Which filament on which plate: PLA, PETG, ABS, TPU, nylon
Choose the surface together with the material. The table summarises general tendencies; the bed temperatures are the typical ranges Bambu Lab publishes for its own plates. For your filament, always check the product's data sheet. The materials themselves are covered in our filament types comparison.
| Material | Good match | Typical bed temperature | Note |
|---|---|---|---|
| PLA | Smooth or textured PEI | About 45–65 °C on PEI | On enclosed printers, open the door |
| PETG | Textured PEI | About 60–80 °C | On smooth PEI, use glue as a release agent |
| ABS / ASA | PEI, engineering plate | About 90–100 °C | Enclosure, brim, no draughts |
| TPU | Textured PEI | About 35–45 °C | Glue is a must on smooth PEI |
| Nylon (PA) | Garolite, glued engineering plate | About 100–120 °C | Dry filament essential; add a brim |
When PETG sticks too well
The bond between PETG and PEI can be stronger than the coating's own hold on the sheet. Pull the part off by force and a flake of PEI can come with it, leaving a permanent mark on the plate. That is why Prusa advises not to wipe smooth PEI with alcohol before PETG and to use a release agent if needed. The simplest answer is a textured plate reserved for PETG. If you must print on smooth PEI, a thin glue layer and patience while the part cools fully will do the job.
PLA in an enclosed printer
PLA softens at a relatively low temperature. In an enclosed printer, heat from the bed warms the chamber and the filament can soften in the extruder and jam. Bambu Lab recommends opening the front door or lifting the top cover for PLA when the bed is above 45 °C.
Nylon and garolite
Nylon grips PEI poorly and absorbs moisture fast. MatterHackers recommends printing it on garolite with a thin layer of PVA glue when extra hold is needed, and gives a bed temperature around 65 °C as its own suggestion. Whatever value you pick, dry filament matters more than the surface.
Warping, brims and mouse ears
Plastic shrinks as it cools. Each new layer contracts on top of a cooler layer below, and the top of the part pulls the bottom inwards. The stress concentrates along long straight edges and in sharp corners, and the moment it exceeds the grip, a corner lifts.
Prusa explains warping as the result of a sudden difference between nozzle and ambient temperature, most visible in high-temperature materials such as ABS, ASA and PC. The fixes fall into two groups: reduce the stress, or enlarge the area holding the part down.
- Calm the environment: keep away from windows and air conditioning. Use an enclosure for ABS and ASA. Without one, PrusaSlicer's draft shield prints a thin wall around the part to keep the air around it a little warmer.
- Brim: a few extra loops around the part on the first layer, enlarging the contact area. Trim it off afterwards.
- Mouse ears: small discs, one or two layers thick, added only at the corners. Less clean-up than a brim, and aimed where the stress gathers.
- Set cooling for the material: on ABS and PC, too much fan encourages cracking and warping.
Clean the surface and fix the first layer first; a brim is no substitute for a sound foundation. For a check order by symptom, see the warping section of our troubleshooting guide.
Removing prints safely
Prising a part off while it is hot damages both the part and the surface. PEI's release only appears as it cools. Bambu Lab also recommends waiting a few minutes until plate and model have fully cooled, then flexing the plate gently to release the part.
- Take the spring steel sheet off and flex it gently in two directions. Never bend it far enough to kink it.
- Use a plastic spatula for small leftovers; a metal scraper scratches PEI.
- If PETG has fused to smooth PEI, do not pull. Let the plate cool fully; a short spell in the fridge can loosen the bond through the temperature difference.
- In a print farm, fix one plate type per material; changing plates also changes the first-layer setting.
Plates are consumables. When the coating turns glossy, starts to lift or adhesion will not come back despite cleaning, replacing the plate is cheaper than hours of tuning. For the choice of material itself, our material selection guide is a good place to start.
Frequently asked questions
Why won't my first layer stick to the bed?
The usual causes are a nozzle set too far from the plate, skin oil on the surface and a first layer printed too fast. Wipe the cold plate with isopropyl alcohol, lower the Z offset in small steps and slow the first layer down. Compare the bed temperature with the filament's data sheet.
Why does PETG stick too well to smooth PEI?
The bond between PETG and PEI can be stronger than the coating's own hold on the sheet, so removing the part can tear the coating. A textured PEI plate, or a thin layer of glue on smooth PEI as a release agent, reduces the risk. Remove the part only once it has fully cooled.
Can I clean a PEI sheet with acetone?
No. Prusa and Bambu Lab both warn that acetone can damage PEI. For everyday cleaning, isopropyl alcohol and a microfibre cloth on a cold plate is enough, with dish soap and water now and then for stubborn residue.
Should I use a brim or mouse ears?
A brim is safer for long, thin parts or when grip is weak all round. Mouse ears need less clean-up on flat parts where the stress gathers only in the corners. Neither replaces a clean surface and a correct first layer.
What is the best build surface for nylon?
Because nylon grips PEI poorly, garolite (G10) or an engineering plate with a thin glue layer is common. Just as important is dry filament: damp nylon prints weak and bubbly on any surface.